A - Unfortunately, there is seldom a quick answer for resolving problems associated with porosity in aluminum welds. The reason for this is that a number of conditions relating to material, consumables, welding technique and / or equipment can cause porosity. It is often necessary to address this problem through a process of elimination, evaluating each of the potential problem areas in order to identify the true cause.
When investigating this type of problem, it is necessary to understand how porosity occurs and how to identify and eliminate these causes.
Porosity is a result of hydrogen gas becoming entrapped within the solidifying aluminum weld puddle and leaving voids in the completed weld. Hydrogen is highly soluble in molten aluminum, and for this reason, the potential for excessive amounts of porosity during arc welding of aluminum is considerably high. During the welding operation, it is easy to introduce Hydrogen unintentionally through contaminants within the welding area. It is important to understand thoroughly the many sources of these contaminants in order to detect the cause and take the necessary action to resolve porosity problems.
Shielding During the Welding Operation
Exposure and contamination of the molten weld metal to the surrounding atmosphere during the welding operation is one consideration when examining a porosity problem. This situation may occur because of inadequate gas shielding during welding. Following are some examples:
Note: By using argon / helium shielding gas mixtures, reduction in porosity level is sometimes achievable. The advantage of the helium mixtures is the ability of this gas to provide additional heat during the welding process, and consequently, provide the hydrogen a greater opportunity to escape prior to solidification. The use of helium as an additive, sometimes up to 75%, can help to provide reduced porosity levels; however, the best line of defense against unacceptable porosity levels is to remove the source of (hydrogen) contamination.
Hydrocarbons
Hydrocarbons are other sources of hydrogen and porosity, which may be present on the surface of the plate or on the welding wire. Following are some examples:
Moisture
Through a number of sources, Moisture (H2O), which contains hydrogen, can also be a source of contamination to the welding area. Following are some examples:
Material Preparation Concerns
Other potential contamination problems are associated with material preparation. Cutting or grinding methods, which may deposit contaminants on to the plate surface or sub-surface, cutting fluids, grinding disc debris, and saw blade lubricants are all areas of concern. Material preparation methods need to be evaluated as controlled elements of the welding procedure and not changed without revalidation. Certain types of grinding discs, for example, can deposit particles within the aluminum that will react during welding and cause major porosity problems. Additionally, aluminum filler material should be stored in an area that will prevent it from becoming contaminated by hydrocarbons or moisture.
Cleaning prior to welding
To achieve low porosity levels for x-ray quality welds, it is important to understand the methods available for the effective removal of hydrocarbons and moisture from the weld area, and to incorporate the appropriate methods into the welding procedure. If these contaminants are present in the weld area during welding, they will produce hydrogen and significantly contribute to porosity problems.
When designing welding procedures intended to produce low levels of porosity, it is important to incorporate degreasing and oxide removal. Typically, you can achieve this through a combination of chemical cleaning and/or the use of solvents to remove hydrocarbons followed by stainless steel wire brushing to remove contaminated aluminum oxide.
Conclusion
Determining the actual cause of porosity within a specific welding operation is not always a straightforward exercise. Without an understanding of the basic principals relating to this problem, it can be an extremely time consuming and often a frustrating process. You must approach a porosity problem from an organized problem-solving standpoint, and work through the possibilities, based on knowledge of the various sources of hydrogen, until finding and eliminating the cause.
The correct cleaning of the aluminum parts prior to welding, use of proven procedures, well maintained equipment, high quality shielding gas, and a high quality aluminum welding wire that is free from contamination, are all very important variables if low porosity levels are desirable.